Home - Education Resources - NDT Course Material - EC Testing
 

-
Eddy Current Testing

Introduction
Basic Principles
History of ET
Present State of ET

The Physics
Properties of Electricity
Current Flow & Ohm's Law
Induction & Inductance
Self Inductance
Mutual Inductance
Circuits & Phase
Impedance
Depth & Current Density
Phase Lag

Instrumentation
Eddy Current Instruments
Resonant Circuits
Bridges
Impedance Plane
Display - Analog Meter

Probes (Coils)
Probes - Mode of Operation
Probes - Configuration
Probes - Shielding
Coil Design
Impedance Matching

Procedures Issues
Reference Standards
Signal Filtering

Applications
Surface Breaking Cracks
SBC using Sliding Probes
Tube Inspection
Conductivity
Heat Treat Verification
Thickness of Thin Mat'ls
Thickness of Coatings

Advanced Techniques
Scanning
Multi-Frequency Tech.
Swept Frequency Tech.
Pulsed ET Tech.
Background Pulsed ET

Remote Field Tech.

Quizzes

Formulae& Tables
EC Standards & Methods
EC Material Properties
-

EC Material Properties

                 CONDUCTIVITY OF MATERIALS SORTED BY NAME
                                 
       Source Code: 1 - CSNDT

                    2 - Eddy Current Testing Manual on Eddy Current Method

                    3 - NDT Magazine Sept/Oct 1955, Cosgrove Article
							
RESIST.   COND,/                   SOURCE

ohm-m     SEIMENS      % IACS      CODE           MATERIAL

-------------------------------------------------------------------------------------------

7.184E-8  1.392E+7	    24.00   2  Admiralty Brass

7.009E-8  1.427E+7	    24.60   1  Admiralty Metal (annealed)

6.386E-8  1.566E+7	    27.00   1  Aluminum Allcast, as cast

4.789E-8  2.088E+7	    36.00   1  Aluminum Allcast, Cond. Sol. H.T. & Stress Relieved

5.747E-8  1.740E+7	    30.00   1  Aluminum Allcast, Sol H.T. and Aged

5.747E-8  1.740E+7	    30.00   1  Aluminum Allcast, Stress Relieved

4.660E-8  2.146E+7	    37.00   1  Aluminum Alloy, A 108

5.945E-8  1.682E+7	    29.00   1  Aluminum Alloy, A 132 Cond. T551

5.225E-8  1.914E+7	    33.00   1  Aluminum Alloy, A214

4.926E-8  2.030E+7	    35.00   1  Aluminum Alloy, B 195 Cond. T4

4.789E-8  2.088E+7	    36.00   1  Aluminum Alloy, B 195 Cond. T6

6.386E-8  1.566E+7	    27.00   1  Aluminum Alloy, C113

6.631E-8  1.508E+7	    26.00   1  Aluminum Alloy, Red X-8 As Cast

5.747E-8  1.740E+7	    30.00   1  Aluminum Alloy, R 317

3.435E-8  2.912E+7  50.10 - 50.30   3  Aluminum Alloy, X3005-0

3.769E-8  2.654E+7  45.50 - 46.00   3  Aluminum Alloy, X7178-F and -0

5.805E-8  1.723E+7  26.80 - 32.60   3  Aluminum Alloy, X7178-W and T6

5.562E-8  1.798E+7	    31.00   1  Aluminum Alloy, 108

2.903E-8  3.445E+7  57.00 - 61.80   3  Aluminum Alloy, 1100

5.747E-8  1.740E+7	    30.00   1  Aluminum Alloy, 113

5.071E-8  1.972E+7	    34.00   1  Aluminum Alloy, 122 Perm. Mold As Cast

4.205E-8  2.378E+7	    41.00   1  Aluminum Alloy, 122 Sand Cond. T2

5.225E-8  1.914E+7	    33.00   1  Aluminum Alloy, 122 Sand Cond. T61

4.421E-8  2.262E+7	    39.00   1  Aluminum Alloy, 13

5.388E-8  1.856E+7	    32.00   1  Aluminum Alloy, 142 Perm. Mold Cond. T61

3.918E-8  2.552E+7	    44.00   1  Aluminum Alloy, 142 Sand Cond. T21

5.071E-8  1.972E+7	    34.00   1  Aluminum Alloy, 142 Sand Cond. T571

4.660E-8  2.146E+7	    37.00   1  Aluminum Alloy, 142 Sand Cond. T77

4.926E-8  2.030E+7	    35.00   1  Aluminum Alloy, 195 Cond. T4

4.660E-8  2.146E+7	    37.00   1  Aluminum Alloy, 195 Cond. T62

4.756E-8  2.103E+7  36.00 - 36.50   3  Aluminum Alloy, 2011-T3

3.473E-8  2.880E+7  48.60 - 50.70   3  Aluminum Alloy, 2014-F and -0

5.124E-8  1.952E+7  32.50 - 34.80   3  Aluminum Alloy, 2014-T3 and -T4

4.438E-8  2.253E+7  38.00 - 39.70   3  Aluminum Alloy, 2014-T6

3.490E-8  2.865E+7  49.30 - 49.50   3  Aluminum Alloy, 2017-F

3.618E-8  2.764E+7  46.80 - 48.50   3  Aluminum Alloy, 2024-F

5.330E-8  1.876E+7  28.60 - 36.10   3  Aluminum Alloy, 2024-T3

5.884E-8  1.699E+7  29.10 - 29.50   3  Aluminum Alloy, 2024-T36

5.766E-8  1.734E+7  28.80 - 31.00   3  Aluminum Alloy, 2024-T4

4.081E-8  2.451E+7  42.10 - 42.40   3  Aluminum Alloy, 2127-T4

4.926E-8  2.030E+7	    35.00   1  Aluminum Alloy, 214

7.184E-8  1.392E+7	    24.00   1  Aluminum Alloy, 218

8.210E-8  1.218E+7	    21.00   1  Aluminum Alloy, 220

4.610E-8  2.169E+7	    37.40   3  Aluminum Alloy, 2218-T61

4.289E-8  2.332E+7	    40.20   3  Aluminum Alloy, 2618

3.861E-8  2.590E+7  37.80 - 51.50   3  Aluminum Alloy, 3003-H14 and -H12

4.043E-8  2.474E+7  37.80 - 47.50   3  Aluminum Alloy, 3003-H24 and -H28

3.649E-8  2.741E+7  44.70 - 49.80   3  Aluminum Alloy, 3003-0

4.160E-8  2.404E+7  39.40 - 43.50   3  Aluminum Alloy, 3004

6.158E-8  1.624E+7	    28.00   1  Aluminum Alloy, 319 Perm. Mold

6.386E-8  1.566E+7	    27.00   1  Aluminum Alloy, 319 Sand

4.421E-8  2.262E+7	    39.00   1  Aluminum Alloy, 355 Perm. Mold Cond. T6

4.010E-8  2.494E+7	    43.00   1  Aluminum Alloy, 355 Sand Cond. T51

4.789E-8  2.088E+7	    36.00   1  Aluminum Alloy, 355 Sand Cond. T6

4.660E-8  2.146E+7	    37.00   1  Aluminum Alloy, 355 Sand Cond. T61

4.105E-8  2.436E+7	    42.00   1  Aluminum Alloy, 355 Sand Cond. T7

4.010E-8  2.494E+7	    43.00   1  Aluminum Alloy, 356 Sand Cond. T51

4.421E-8  2.262E+7	    39.00   1  Aluminum Alloy, 356 Sand Cond. T6

4.660E-8  2.146E+7	    37.00   1  Aluminum Alloy, 360

6.386E-8  1.566E+7	    27.00   1  Aluminum Alloy, 380

4.926E-8  2.030E+7	    35.00   1  Aluminum Alloy, 40E

4.816E-8  2.076E+7  35.30 - 36.30   3  Aluminum Alloy, 4032-T6

3.235E-8  3.091E+7  52.30 - 54.30   3  Aluminum Alloy, 4043-F

4.105E-8  2.436E+7	    42.00   1  Aluminum Alloy, 43 (Annealed)

4.660E-8  2.146E+7	    37.00   1  Aluminum Alloy, 43 As Cast

3.281E-8  3.048E+7  52.30 - 52.80   3  Aluminum Alloy, 5005

3.515E-8  2.845E+7  48.30 - 49.80   3  Aluminum Alloy, 5050

4.843E-8  2.065E+7  33.60 - 37.60   3  Aluminum Alloy, 5052

5.956E-8  1.679E+7  28.10 - 29.80   3  Aluminum Alloy, 5056

5.448E-8  1.836E+7  30.50 - 32.80   3  Aluminum Alloy, 5154

3.861E-8  2.590E+7  42.30 - 47.00   3  Aluminum Alloy, 5357

3.950E-8  2.532E+7  39.30 - 48.00   3  Aluminum Alloy, 6053

3.798E-8  2.633E+7  42.30 - 48.50   3  Aluminum Alloy, 6061-F and -0

4.415E-8  2.265E+7  37.60 - 40.50   3  Aluminum Alloy, 6061-T4

4.066E-8  2.459E+7  40.00 - 44.80   3  Aluminum Alloy, 6061-T6 and -T9

3.519E-8  2.842E+7  47.00 - 51.00   3  Aluminum Alloy, 6062-F

3.941E-8  2.538E+7  43.50 - 44.00   3  Aluminum Alloy, 6062-T4

3.661E-8  2.732E+7  44.70 - 49.50   3  Aluminum Alloy, 6062-T6

4.066E-8  2.459E+7  41.50 - 43.30   3  Aluminum Alloy, 6151-T4

3.879E-8  2.578E+7  43.90 - 45.00   3  Aluminum Alloy, 6151-T6

3.184E-8  3.141E+7  53.30 - 55.00   3  Aluminum Alloy, 6151-0

3.250E-8  3.077E+7  53.00 - 53.10   3  Aluminum Alloy, 6951-F

3.073E-8  3.254E+7  55.70 - 56.50   3  Aluminum Alloy, 6951-0

2.871E-8  3.483E+7  60.00 - 60.10   3  Aluminum Alloy, 7072

3.736E-8  2.677E+7  44.50 - 47.80   3  Aluminum Alloy, 7075-F

5.209E-8  1.920E+7  31.40 - 34.80   3  Aluminum Alloy, 7075-T6

5.388E-8  1.856E+7	    32.00   2  Aluminum Alloy, 7075-T6

5.388E-8  1.856E+7  27.00 - 37.00   3  Aluminum Alloy, 7075-W

3.831E-8  2.610E+7	    45.00   1  Aluminum Alloy, 750

6.158E-8  1.624E+7	    28.00   1  Aluminum Alloy, 85

3.135E-8  3.190E+7	    55.00   1  Aluminum, A51S Cond. "0"

3.831E-8  2.610E+7	    45.00   1  Aluminum, A51S Cond. T4 and T6

7.496E-8  1.334E+7	    23.00   1  Aluminum Brass (Annealed)

1.232E-7  8.120E+6	    14.00   1  Aluminum - Bronze

9.852E-8  1.015E+7	    17.50   1  Aluminum - Bronze, 5% Aluminum (Annealed)

1.368E-7  7.308E+6	    12.60   1  Aluminum - Bronze, 10% Aluminum (Annealed)

2.826E-8  3.538E+7	    61.00   2  Aluminum, Pure

5.945E-8  1.682E+7	    29.00   1  Aluminum, Red X-8 Cond. Stress Relieved

4.310E-8  2.320E+7	    40.00   1  Aluminum, 11S Cond. T3

3.448E-8  2.900E+7	    50.00   1  Aluminum, 14S Cond. "0"

4.310E-8  2.320E+7	    40.00   1  Aluminum, 14S Cond. T6

3.831E-8  2.610E+7	    45.00   1  Aluminum, 17S Cond. "0"

5.747E-8  1.740E+7	    30.00   1  Aluminum, 17S Cond. T4

3.448E-8  2.900E+7	    50.00   1  Aluminum, 18S Cond. "0"

4.310E-8  2.320E+7	    40.00   1  Aluminum, 18S Cond. T61

2.922E-8  3.422E+7	    59.00   1  Aluminum, 2S Cond. "0"

3.025E-8  3.306E+7	    57.00   1  Aluminum, 2S Cond. H18

3.448E-8  2.900E+7	    50.00   1  Aluminum, 24S Cond. "0"

5.747E-8  1.740E+7	    30.00   1  Aluminum, 24S Cond. T4

4.310E-8  2.320E+7	    40.00   1  Aluminum, 24S Cond. T6

3.448E-8  2.900E+7	    50.00   1  Aluminum, 3S Cond. "0"

4.105E-8  2.436E+7	    42.00   1  Aluminum, 3S Cond. H 12

4.205E-8  2.378E+7	    41.00   1  Aluminum, 3S Cond. H 14

4.310E-8  2.320E+7	    40.00   1  Aluminum, 3S Cond. H 18

4.310E-8  2.320E+7	    40.00   1  Aluminum, 32S Cond. "0"

4.926E-8  2.030E+7	    35.00   1  Aluminum, 32S Cond. T6

4.926E-8  2.030E+7	    35.00   1  Aluminum, 52S Cond. "0" and H 38

3.831E-8  2.610E+7	    45.00   1  Aluminum, 53S Cond. "0"

4.310E-8  2.320E+7	    40.00   1  Aluminum, 53S Cond. T4 and T6

5.945E-8  1.682E+7	    29.00   1  Aluminum, 56S Cond. "0"

3.831E-8  2.610E+7	    45.00   1  Aluminum, 61S Cond. "0"

6.386E-8  1.566E+7	    27.00   1  Aluminum, 56S Cond. H 38

4.310E-8  2.320E+7	    40.00   1  Aluminum, 61S Cond. T4 and T6

5.747E-8  1.740E+7	    30.00   1  Aluminum, 75S Cond. T6

2.655E-8  3.767E+7	    64.94   1  Aluminum, 99.99%

1.449E-7  6.902E+6	    11.90   1  Antimonial Tin Solder

2.188E-7  4.570E+6	     7.88   1  Antimonial Lead, 1% (Quenched and Aged)

3.918E-7  2.552E+6	     4.40   1  Antimony

2.874E-7  3.480E+6	     6.00   1  Babbit, Lead Base

1.014E-7  9.860E+6	    17.00   1  Beryllium Copper, Cond. A

8.210E-8  1.218E+7	    21.00   1  Beryllium Copper, Cond. At

4.000E-8  2.500E+7	    43.10   1  Beryllium

4.432E-8  2.256E+7	    38.90   1  Beryllium

7.184E-8  1.392E+7	    24.00   2  Brass, Admiralty

7.496E-8  1.334E+7	    23.00   1  Brass, Aluminum (Annealed)

6.158E-8  1.624E+7	    28.00   1  Brass, Cartridge (Annealed)

1.437E-7  6.960E+6	    12.00   1  Brass, High Strength Yellow

6.631E-8  1.508E+7	    26.00   1  Brass, Leaded Naval (Annealed)

9.579E-8  1.044E+7	    18.00   1  Brass, Leaded Semi Red

6.897E-8  1.450E+7	    25.00   1  Brass, Leaded Yellow

5.388E-8  1.856E+7	    32.00   1  Brass, Low (Annealed)

6.631E-8  1.508E+7	    26.00   1  Brass, Low Leaded (Annealed)

6.631E-8  1.508E+7	    26.00   1  Brass, Naval (Annealed)

4.660E-8  2.146E+7	    37.00   1  Brass, Red (Annealed)

6.386E-8  1.566E+7	    27.00   1  Brass, Yellow (Annealed)

1.232E-7  8.120E+6	    14.00   1  Bronze Aluminum

9.852E-8  1.015E+7	    17.50   1  Bronze Aluminum, 5% Aluminum (Annealed)

1.368E-7  7.308E+6	    12.60   1  Bronze Aluminum, 10% Aluminum (Annealed)

3.918E-8  2.552E+7	    44.00   1  Bronze, Commercial (Annealed)

4.105E-8  2.436E+7	    42.00   1  Bronze, Commercial Leaded

1.567E-7  6.380E+6	    11.00   2  Bronze, Phos.

1.232E-7  8.120E+6	    14.00   1  Bronze, Leaded Tin

1.567E-7  6.380E+6	    11.00   1  Bronze, Leaded Tin Bearing

7.184E-8  1.392E+7	    24.00   1  Bronze Manganese (Annealed)

3.592E-8  2.784E+7	    48.00   1  Bronze Phos., 1.25% Phos. Grade E

9.579E-8  1.044E+7	    18.00   1  Bronze Phos., 5% Phos. Grade A

1.326E-7  7.540E+6	    13.00   1  Bronze Phos., 8% Phos. Grade C

1.567E-7  6.380E+6	    11.00   1  Bronze Phos., 10% Phos. Grade D

2.463E-7  4.060E+6	     7.00   1  Bronze, Silicon Type A (Annealed)

1.437E-7  6.960E+6	    12.00   1  Bronze, Silicon Type B (Annealed)

6.842E-8  1.462E+7	    25.20   1  Cadmium

3.540E-8  2.825E+7	    48.70   1  Calcium

6.158E-8  1.624E+7	    28.00   1  Cartridge Brass (Annealed)

1.959E-7  5.104E+6	     8.80   1  Chromium

6.247E-8  1.601E+7	    27.60   1  Cobalt

1.306E-7  7.656E+6	    13.20   1  Columbium

4.898E-7  2.042E+6	     3.52   1  Constantan

1.014E-7  9.860E+6	    17.00   1  Copper Beryllium, Cond. "A"

8.210E-8  1.218E+7	    21.00   1  Copper Beryllium, Cond. At

2.028E-8  4.930E+7	    85.00   1  Copper, Deoxidized (Annealed)

1.707E-8  5.858E+7	   101.00   1  Copper, Electrolytic Tough Pitch (Annealed)

1.664E-8  6.009E+7	   103.60   1  Copper, Pure

1.724E-8  5.800E+7	   100.00   2  Copper, Pure

3.831E-7  2.610E+6	     4.50   2  Copper 70%, Nickel 30%

1.771E-7  5.647E+6	     9.74   4  Copper 90%, Nickel 10%

2.077E-7  4.814E+6	     8.30   1  Corrodine Lead

3.748E-7  2.668E+6	     4.60   1  Cupro - Nickel 30%

3.079E-8  3.248E+7	    56.00   1  Gilding Metal (Annealed)

2.349E-8  4.257E+7	    73.40   1  Gold

2.463E-8  4.060E+7	    70.00   2  Gold, Pure

7.837E-6  1.276E+5	     0.22   1  Graphite

1.232E-6  8.120E+5	     1.40   1  Hastelloy "A"

1.326E-6  7.540E+5	     1.30   1  Hastelloy "B" & "C"

1.149E-6  8.700E+5	     1.50   1  Hastelloy "D"

1.149E-6  8.700E+5	     1.50   2  Hastelloy "X"

9.796E-7  1.021E+6	     1.76   1  Inconel

1.014E-6  9.860E+5	     1.70   2  Inconel 600

1.105E-7  9.048E+6	    15.60   1  Ingot Iron (99.9% Fe)

5.289E-8  1.891E+7	    32.60   1  Iridium

1.895E-7  5.278E+6	     9.10   1  Iridium - Platinum Alloys

3.316E-7  3.016E+6	     5.20   1  Iridium - Platinum Alloys, 18% Nickel Silver Alloy B

9.579E-8  1.044E+7	    18.00   2  Iron

1.105E-7  9.048E+6	    15.60   1  Iron Ignot (99.9% Fe)

2.053E-7  4.872E+6	     8.40   2  Lead

2.188E-7  4.570E+6	     7.88   1  Lead, 1% Antimonial (Quenched & Aged)

2.077E-7  4.814E+6	     8.30   1  Lead, Corrodine

2.239E-7  4.466E+6	     7.70   1  Lead, Hard (Quenched & Aged)

4.105E-8  2.436E+7	    42.00   1  Leaded Commercial Bronze

9.579E-8  1.044E+7	    18.00   1  Leaded Semi Red Brass

1.567E-7  6.380E+6	    11.00   1  Leaded Tin Bearing Bronze

1.232E-7  8.120E+6	    14.00   1  Leaded Tin Bronze

6.897E-8  1.450E+7	    25.00   1  Leaded Yellow Brass

8.535E-8  1.172E+7	    20.20   1  Lithium

4.660E-8  2.146E+7	    37.00   2  Magnesium

1.149E-7  8.700E+6	    15.00   1  Magnesium Alloys (Cast)

1.596E-7  6.264E+6	    10.80   1  Magnesium, AZ80BTA

1.916E-7  5.220E+6	     9.00   1  Magnesium Cast Alloys

1.181E-7  8.468E+6	    14.60   1  Magnesium, A2 80

1.002E-7  9.976E+6	    17.20   1  Magnesium, A231

1.347E-7  7.424E+6	    12.80   1  Magnesium, A251

1.402E-7  7.134E+6	    12.30   1  Magnesium, A261

4.467E-8  2.239E+7	    38.60   1  Magnesium, Pure

1.379E-7  7.250E+6	    12.50   1  Magnesium, T454

4.998E-8  2.001E+7	    34.50   1  Magnesium (Wrought Alloys)

7.184E-8  1.392E+7	    24.00   1  Manganese Bronze (Annealed)

5.225E-8  1.914E+7	    33.00   1  Molybdenum

4.789E-7  2.088E+6	     3.60   2  Monel

4.816E-7  2.076E+6	     3.58   1  Monel

9.579E-7  1.044E+6	     1.80   1  Mercury

6.158E-8  1.624E+7	    28.00   1  Muntz Metal (Annealed)

3.831E-7  2.610E+6	     4.50   2  Nickel 30%, Copper 70%

9.579E-8  1.044E+7	    18.00   1  Nickel "A"

2.330E-7  4.292E+6	     7.40   1  Nickel - Platinum Alloys

1.268E-7  7.888E+6	    13.60   1  Nickel - Platinum Alloys

6.842E-8  1.462E+7	    25.20   1  Nickel, Pure (Electrolytic)

3.748E-7  2.668E+6	     4.60   1  Nickel 30% - Cupro

2.874E-7  3.480E+6	     6.00   1  Nickel, 18% Nickel Sil

9.473E-8  1.056E+7	    18.20   1  Osmium

1.078E-7  9.280E+6	    16.00   1  Palladium

1.567E-7  6.380E+6	    11.00   2  Phos. Bronze

3.592E-8  2.784E+7	    48.00   1  Phos. Bronze, 1.25% Phos. Grade E

9.579E-8  1.044E+7	    18.00   1  Phos. Bronze, 5% Phos. Grade A

1.326E-7  7.540E+6	    13.00   1  Phos. Bronze, 8% Phos. Grade C

1.567E-7  6.380E+6	    11.00   1  Phos. Bronze, 10% Phos. Grade D

1.059E-7  9.442E+6	    16.28   1  Platinum

1.486E-7  6.728E+6	    11.60   1  Platinum, Commercial

1.895E-7  5.278E+6	     9.10   1  Platinum - Iridium Alloys

3.316E-7  3.016E+6	     5.20   1  Platinum - Iridium Alloys, 18% Nickel Silver Alloy B

2.330E-7  4.292E+6	     7.40   1  Platinum - Nickel Alloys

1.268E-7  7.888E+6	    13.60   1  Platinum - Nickel Alloys

4.310E-7  2.320E+6	     4.00   1  Platinum - Ruthenium (Contact Grade)

3.135E-7  3.190E+6	     5.50   1  Platinum - Ruthenium (Jewelry Grade)

4.490E-8  2.227E+7	    38.40   1  Rhodium

7.595E-8  1.317E+7	    22.70   1  Ruthenium

4.310E-7  2.320E+6	     4.00   1  Ruthenium - Platinum (Contact Grade)

3.135E-7  3.190E+6	     5.50   1  Ruthenium - Platinum (Jewelry Grade)

1.197E-7  8.352E+6	    14.40   1  Selenium

2.463E-7  4.060E+6	     7.00   1  Silicon Bronze, Type A (Annealed)

1.437E-7  6.960E+6	    12.00   1  Silicon Bronze, Type B (Annealed)

1.642E-8  6.090E+7	   105.00   2  Silver, Pure

1.591E-8  6.287E+7	   108.40   1  Silver, Pure

1.039E-7  9.628E+6	    16.60   1  Silver, Tin Solder

2.874E-7  3.480E+6	     6.00   1  Silver, 18% Nickel Alloy A

1.449E-7  6.902E+6	    11.90   1  Solder, Antimonial Tin

1.039E-7  9.628E+6	    16.60   1  Solder, Tin Silver

1.759E-7  5.684E+6	     9.80   1  Solder, 20-80 Soft

1.959E-7  5.104E+6	     8.80   1  Solder, 5-95 Soft

1.567E-7  6.380E+6	    11.00   1  Solder, 50-50 Soft

1.611E-7  6.206E+6	    10.70   1  Steel, Cast

5.945E-7  1.682E+6	     2.90   1  Steel, High Alloy

6.897E-7  1.450E+6	     2.50   2  Steel, 304 Stainless

6.897E-7  1.450E+6	     2.50   1  Steel, 304 Stainless

7.496E-7  1.334E+6	     2.30   1  Steel, 316 Stainless

7.184E-7  1.392E+6	     2.40   1  Steel, 347 Stainless

1.240E-7  8.062E+6	    13.90   1  Tantalum

1.449E-7  6.902E+6	    11.90   1  Tin Solder (Antimonial)

4.105E-7  2.436E+6	     4.20   1  Tin, Foil

1.232E-7  8.120E+6	    14.00   1  Tin (Leaded), Bronze

1.149E-7  8.700E+6	    15.00   1  Tin, Pure

1.039E-7  9.628E+6	    16.60   1  Tin, Silver Solder

5.562E-7  1.798E+6	     3.10   2  Titanium

7.837E-7  1.276E+6	     2.20   1  Titanium

1.724E-6  5.800E+5	     1.00   2  Titanium, 6AL-4V

5.491E-8  1.821E+7	    31.40   1  Tungsten

2.874E-7  3.480E+6	     6.00   1  Uranium

2.612E-7  3.828E+6	     6.60   1  Vanadium

1.232E-6  8.120E+5	     1.40   2  Waspaloy

1.553E-7  6.438E+6	    11.10   1  White Metal

5.945E-8  1.682E+7	    29.00   2  Zinc

6.158E-8  1.624E+7	    28.00   1  Zinc, Commercial Rolled

6.897E-8  1.450E+7	    25.00   1  Zinc, Die Cast

6.386E-8  1.566E+7	    27.00   1  Zinc, Die Cast

7.184E-7  1.392E+6	     2.40   2  Zircaloy - 2

4.105E-7  2.436E+6	     4.20   1  Zirconium

5.071E-7  1.972E+6	     3.40   2  Zirconium