Home - General Resources - Material Properties Tables - UT
Piezoelectrics
Longitudinal Velocity (cm/µsec)
e R,
(10-12m/v)
(10-3vm/n)
AlN
.488
N/A
2440
8.8
42.94
Barium Titanate
.564
1200
149
14.1
2740
5.55
33.5
Lead Zirconate Titanate
PZT-2
.441
450
152
38.1
2090
7.6
31.3
PZT-4
.460
1300
289
26.1
2000
7.5
34.5
PZT-5A
.435
1700
380
24.8
1890
7.75
33.7
PZT-5H
.456
3400
593
19.7
34.2
K180
.400
425
180
41
2006
7.7
31
K270
.406
270
26
2032
K278
1100
240
K350
.396
290
25
1981
30.5
K500
2700
500
20
K550
.408
3000
550
7.8
Lead Titanate
K NTA
.417
170
62
40
2082
33
K N3B
.427
215
70
37
2134
7.65
Lead Metanlobate
K-81
.305
300
85
32
1524
6.2
19
K-83
.548
175
65
42
2743
4.5
24.5
K-85
.335
80
27
1676
5.7
18.5
PVDF
.220
12
339
1.78
2.5
Lithium Niobate
(Z-cut)
.773
4.64
34.0
(Y-cut)
.688
31.9
Sodium Bismuth Titanate
140
18
15
K15
7.2
29
Lithium Sulfate (Y-cut)
.546
10.3
165
2730
2.06
11.2
Quartz
.566
2.3
2830
6.82
15.2
Tourmaline
.754
3770
3.1
23.4
Data compiled by Xactex Corporation. Sources of original data are unknown.
-