| Material |
Conductivity
|
Resistivity
|
Reference
|
Notes |
|
(% IACS)
|
(Siemens/m)
|
(Ohm-m)
|
(See Below)
|
|
| Copper
and Alloys by Copper Alloy Number
|
|
|
|
|
|
| Pure (annealed) |
100.00
|
5.800E+07
|
1.724E-08
|
ECTM
|
|
| C10100, C10200 |
101.00
|
|
1.710E-08
|
MHASM2
|
|
| C10300-O61 |
99.00
|
|
1.740E-08
|
MHASM2
|
|
| C10400, C10500, C10700 (O61 temper) |
100.00
|
|
1.720E-08
|
MHASM2
|
|
| C10800-O61 |
92.00
|
|
1.870E-08
|
MHASM2
|
|
| C11000-O60 |
100-101.5
|
|
1.700E-8--1.724E-8
|
MHASM2
|
|
| C11000-H14 |
97.00
|
|
1.780E-08
|
MHASM2
|
|
| C11100 |
100.00
|
|
1.720E-08
|
MHASM2
|
|
| C11300, C11400, C11500, C11600 |
100.00
|
|
1.720E-08
|
MHASM2
|
|
| C12500, C12700, C12800, C12900, C13000 (annealed) |
98.00
|
|
1.760E-08
|
MHASM2
|
|
| C14300 |
96.00
|
|
1.800E-08
|
MHASM2
|
|
| C14310 |
85.00
|
|
2.030E-08
|
MHASM2
|
|
| C14500 |
93.00
|
|
1.860E-08
|
MHASM2
|
|
| C14700-O61 |
95.00
|
|
1.810E-08
|
MHASM2
|
|
| C15000 |
93.00
|
|
1.860E-08
|
MHASM2
|
|
| C15100 (annealed) |
95.00
|
|
1.810E-08
|
MHASM2
|
|
| C15100 (rolled) |
90.00
|
|
1.920E-08
|
MHASM2
|
|
| C15500 (annealed) |
91.00
|
|
1.900E-08
|
MHASM2
|
|
| C15710 |
90.00
|
|
1.920E-08
|
MHASM2
|
|
| C15720 |
89.00
|
|
1.940E-08
|
MHASM2
|
|
| C16200 |
90.00
|
|
1.920E-08
|
MHASM2
|
|
| C17000-TB00 (strip) |
28-33
|
|
5.2E-8--6.2E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TB00 (rod, bar, plate tubing, forgings) |
17-19
|
|
9.1E-8--1.0E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TB00 (billet) |
13-18
|
|
9.6E-8--1.3E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD01 (strip) |
29-34
|
|
5.0E-8--5.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD02 (strip) |
32-38
|
|
4.5E-8--5.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD04 (strip) |
35-39
|
|
4.4E-8--4.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD04 (rod, bar, plate tubing) |
15-17
|
|
1.0E-7--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TF00 (strip) |
35-39
|
|
4.8E-8--4.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TF00 (rod, bar, plate tubing, forgings) |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TF00 (billet) |
18-25
|
|
6.9E-8--9.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH01 (strip) |
36-41
|
|
4.1E-8--4.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH02 (strip) |
36-42
|
|
3.8E-8--4.5E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH04 (strip) |
38-45
|
|
4.7E-8--5.2E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH04 (rod, bar, plate tubing) |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM00 (strip) |
33-37
|
|
4.5E-8--5.1E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM01 (strip) |
34-38
|
|
4.4E-8--4.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM02 (strip) |
35-39
|
|
4.3E-8--4.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM04 (strip) |
36-40
|
|
4.1E-8--4.7E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM06 (strip) |
37-42
|
|
4.1E-8--4.7E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM08 (strip) |
33-45
|
|
3.8E-8--5.2E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000 as-cast (billet) |
16-22
|
|
7.8E-8--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000 cast and aged (billet) |
18-23
|
|
7.5E-8--9.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TB00 |
17-19
|
|
9.1E-8--1.0E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TB00 (billets) |
25-45
|
|
3.8E-8--6.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TD01 |
16-18
|
|
9.6E-8--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TD02 |
15-17
|
|
1.0E-7--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TD04 |
15-17
|
|
1.0E-7--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TF00 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TF00 (billets) |
1.0-3.0
|
|
5.7E-7--1.7E-6
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TH01 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TH02 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TH04 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM00 |
20-28
|
|
6.2E-8--8.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM01 |
20-28
|
|
6.2E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM02 |
20-28
|
|
6.2E-8--8.6E-10
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM04 |
20-28
|
|
6.2E-8--8.6E-11
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM06 |
20-28
|
|
6.2E-8--8.6E-12
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM08 |
20-28
|
|
6.2E-8--8.6E-13
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300 as-cast (billet) |
15-30
|
|
5.7E-8--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300 cast and aged (billet) |
10.0-20
|
|
8.6E-8--1.7E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17410 |
45.00
|
|
3.800E-08
|
MHASM2
|
|
| C17500-TB00 |
20-30
|
|
5.7E-8--8.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-H04 |
20-30
|
|
5.7E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-TF00 |
45-60
|
|
2.9E-8--3.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-TH04 |
50-60
|
|
2.9E-8--3.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-HTR |
45-60
|
|
2.9E-8--3.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-HTC |
60 min
|
|
2.9E-8 max
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TB00 |
20-30
|
|
5.7E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TB00 (billet) |
22-28
|
|
6.2E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-H04 |
20-30
|
|
5.7E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TF00 |
45-60
|
|
2.9E-8--3.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TF00 (billet, forged products) |
50-60
|
|
2.9E-8--3.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TH04 |
50-60
|
|
2.9E-8--3.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600 as-cast (billet) |
32-37
|
|
4.7E-8--5.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600 cast and aged (billet) |
40-50
|
|
3.4E-8--4.3E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C18100 (annealed) |
80.00
|
|
2.170E-08
|
MHASM2
|
|
| C18200, C18400, C18500-TB00 |
40.00
|
|
4.310E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C18200, C18400, C18500-TH04 |
80.00
|
|
2.163E-08
|
MHASM2
|
|
| C18700 |
96.00
|
|
7.790E-08
|
MHASM2
|
|
| C19200 (strip) |
60.00
|
|
2.880E-08
|
MHASM2
|
|
| C19200 (tubing) |
50.00
|
|
3.450E-08
|
MHASM2
|
|
| C19210 |
80.00
|
|
2.160E-08
|
MHASM2
|
|
| C19400-O60 |
40.00
|
|
4.310E-08
|
MHASM2
|
|
| C19400-H14 |
50.00
|
|
3.450E-08
|
MHASM2
|
|
| C19400 (all other tempers) |
65 nominal
|
|
2.26e-8 nominal
|
MHASM2
|
|
| C19500 |
50.00
|
|
3.440E-08
|
MHASM2
|
|
| C19520 |
40.00
|
|
4.930E-08
|
MHASM2
|
|
| C19700 |
80.00
|
|
2.160E-08
|
MHASM2
|
|
| C21000 (annealed) |
56.00
|
|
3.100E-08
|
MHASM2
|
|
| C22000 (annealed) |
44.00
|
|
3.910E-08
|
MHASM2
|
|
| C22600 (annealed) |
40.00
|
|
4.300E-08
|
MHASM2
|
|
| C23000 (annealed) |
37.00
|
|
4.700E-08
|
MHASM2
|
|
| C24000-O61 |
32.00
|
|
5.400E-08
|
MHASM2
|
|
| C26000-O61 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C26800, C27000 (annealed) |
27.00
|
|
6.400E-08
|
MHASM2
|
|
| C28000 |
28.00
|
|
6.160E-08
|
MHASM2
|
|
| C31400 |
42.00
|
|
4.100E-08
|
MHASM2
|
|
| C31600 |
32.00
|
|
5.400E-08
|
MHASM2
|
|
| C33000 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C33200-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C33500 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C34000-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C34200, C35300-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C34900 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C35000 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C35600-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C36000-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C36500, C36600, C36700, C36800-O61 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C37000-O61 |
27.00
|
|
6.390E-08
|
MHASM2
|
|
| C37700 |
27.00
|
|
6.400E-08
|
MHASM2
|
|
| C38500-O61 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C40500 |
41.00
|
|
4.200E-08
|
MHASM2
|
|
| C40800 |
37.00
|
|
4.660E-08
|
MHASM2
|
|
| C41100 |
32.00
|
|
5.400E-08
|
MHASM2
|
|
| C41500 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C41900 |
22.00
|
|
7.800E-08
|
MHASM2
|
|
| C42200 |
31.00
|
|
5.500E-08
|
MHASM2
|
|
| C42500 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C43000 |
27.00
|
|
6.400E-08
|
MHASM2
|
|
| C43400 |
31.00
|
|
5.600E-08
|
MHASM2
|
|
| C43500 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C44300, C44400, C44500 |
25.00
|
|
6.900E-08
|
MHASM2
|
|
| C46400, C45600, C46600, C46700 (annealed) |
26.00
|
|
6.630E-08
|
MHASM2
|
|
| C48200 |
26.00
|
|
6.630E-08
|
MHASM2
|
|
| C48500 |
26.00
|
|
6.630E-08
|
MHASM2
|
|
| C50500 |
48.00
|
|
3.600E-08
|
MHASM2
|
|
| C50710 |
30.00
|
|
5.740E-08
|
MHASM2
|
|
| C51000 |
20.00
|
|
8.700E-08
|
MHASM2
|
|
| C51100 |
20.00
|
|
8.700E-08
|
MHASM2
|
|
| C52100 |
13.00
|
|
1.330E-07
|
MHASM2
|
|
| C52400 |
11.00
|
|
1.570E-07
|
MHASM2
|
|
| C54400 |
19.00
|
|
9.100E-08
|
MHASM2
|
|
| C60600 |
17.00
|
|
1.000E-07
|
MHASM2
|
|
| C60800 |
17.00
|
|
1.000E-07
|
MHASM2
|
|
| C61000 |
15.00
|
|
1.150E-08
|
MHASM2
|
|
| C61300 |
12.00
|
|
1.440E-07
|
MHASM2
|
|
| C61400 |
14.00
|
|
1.230E-07
|
MHASM2
|
|
| C61500 |
12.60
|
|
1.370E-07
|
MHASM2
|
|
| C62300 |
12.00
|
|
1.440E-07
|
MHASM2
|
|
| C62400 |
12.00
|
|
1.440E-07
|
MHASM2
|
|
| C62500 |
10.00
|
|
1.720E-07
|
MHASM2
|
|
| C63000 |
9.00
|
|
1.920E-06
|
MHASM2
|
|
| C63200 |
7.00
|
|
2.460E-08
|
MHASM2
|
|
| C63600 |
12.00
|
|
1.430E-07
|
MHASM2
|
|
| C63800 |
10.00
|
|
1.740E-07
|
MHASM2
|
|
| C65100 |
12.00
|
|
1.440E-07
|
MHASM2
|
|
| C65400 |
7.00
|
|
2.460E-07
|
MHASM2
|
|
| C65500 |
7.00
|
|
2.460E-07
|
MHASM2
|
|
| C66400-O61 |
30.00
|
|
5.750E-08
|
MHASM2
|
|
| C68800-O61 |
18.00
|
|
9.600E-08
|
MHASM2
|
|
| C68800-H08 |
16.60
|
|
1.040E-07
|
MHASM2
|
|
| C69000-O61 |
18.00
|
|
9.600E-08
|
MHASM2
|
|
| C69400 |
6.20
|
|
2.800E-07
|
MHASM2
|
|
| C70250 |
35-40
|
|
4.31E-8--4.93E-8
|
MHASM2
|
|
| C70400 |
14.00
|
|
1.200E-07
|
MHASM2
|
|
| C70600 |
9.10
|
|
1.900E-07
|
MHASM2
|
|
| C71000-O61 |
6.50
|
|
2.650E-07
|
MHASM2
|
|
| C71500-O61 |
4.60
|
|
3.750E-07
|
MHASM2
|
|
| C71900 |
4.40
|
|
3.950E-07
|
MHASM2
|
|
| C72200 |
6.53
|
|
2.640E-07
|
MHASM2
|
|
| C72500 |
11.00
|
|
1.570E-07
|
MHASM2
|
|
| C74500 |
9.00
|
|
1.920E-07
|
MHASM2
|
|
| C75200 |
6.00
|
|
2.870E-07
|
MHASM2
|
|
| C75400 |
7.00
|
|
2.460E-07
|
MHASM2
|
|
| C75700 |
8.00
|
|
2.160E-07
|
MHASM2
|
|
| C77000 |
5.50
|
|
3.140E-07
|
MHASM2
|
|
| C78200 |
10.90
|
|
1.600E-07
|
MHASM2
|
|
| C81100 |
92.00
|
|
1.874E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C81300 |
60.00
|
|
2.874E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C81500 (solution heat treated) |
40-50
|
|
3.830E-08
|
MHASM2
|
|
| C81500 (precipitation hardened) |
80-90
|
|
2.100E-08
|
MHASM2
|
|
| C81800 |
48.00
|
|
3.590E-08
|
MHASM2
|
|
| C82000 |
48.00
|
|
3.590E-08
|
MHASM2
|
|
| C82200 |
48.00
|
|
3.590E-08
|
MHASM2
|
|
| C82400 |
25.00
|
|
6.900E-08
|
MHASM2
|
|
| C82500 |
20.00
|
|
8.620E-08
|
MHASM2
|
|
| C82600 |
19.00
|
|
9.070E-08
|
MHASM2
|
|
| C82800 |
18.00
|
|
9.580E-08
|
MHASM2
|
|
| C83300 |
32.00
|
|
5.388E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C83600 |
15.00
|
|
1.149E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C83800 |
15.00
|
|
1.149E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C84400 |
16.40
|
|
1.051E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C84800 |
16.40
|
|
1.051E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C85200 |
18.60
|
|
9.269E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C85400 |
19.60
|
|
8.796E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C85700, C85800 |
22.00
|
|
7.837E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C86100, C86200 |
7.50
|
|
2.299E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C86300 |
9.00
|
|
1.916E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C86400 |
22.00
|
|
7.837E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C86500 |
20.50
|
|
8.410E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C86700 |
32.00
|
|
5.388E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C86800 |
9.00
|
|
1.916E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C87300 (formerly C87200) |
6.70
|
|
2.573E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C87600 |
6.00
|
|
2.874E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C87500, C87800 |
6.70
|
|
2.840E-07
|
MHASM2
|
|
| C87900 |
15.00
|
|
1.149E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C90300 |
12.00
|
|
1.437E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C90500 |
11.00
|
|
1.567E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C90700 |
9.60
|
|
1.500E-08
|
MHASM2
|
|
| C91700 |
10.00
|
|
1.724E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C92200 |
14.30
|
|
1.200E-07
|
MHASM2
|
|
| C92300 |
12.00
|
|
1.437E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C92600 |
9.00
|
|
1.916E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C92700 |
11.00
|
|
1.567E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C92900 |
9.20
|
|
1.874E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C93200 |
12.00
|
|
1.437E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C93400 |
12.00
|
|
1.437E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C93500 |
15.00
|
|
1.149E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C93700 |
10.14
|
|
1.700E-07
|
MHASM2
|
conductivty
converted from resistivity |
| C93800 |
11.50
|
|
1.499E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C93900 |
11.50
|
|
1.499E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C94300 |
9.00
|
|
1.916E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C94500 |
10.00
|
|
1.724E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C95200 |
12.00
|
|
1.440E-07
|
MHASM2
|
|
| C95300 |
13.00
|
|
1.330E-07
|
MHASM2
|
|
| C95400 |
13.00
|
|
1.330E-07
|
MHASM2
|
|
| C95500 |
8.50
|
|
2.030E-07
|
MHASM2
|
|
| C95600 |
8.50
|
|
2.028E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C95700 |
3.10
|
|
5.560E-07
|
MHASM2
|
|
| C95800 |
7.10
|
|
2.430E-07
|
MHASM2
|
|
| C96200 |
11.00
|
|
1.567E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C96400 |
5.00
|
|
3.448E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C96600 |
4.30
|
|
4.000E-09
|
MHASM2
|
|
| C97300 (as-cast) |
5.70
|
|
3.025E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C97600 (as-cast) |
5.00
|
|
3.448E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C97800 (as-cast) |
4.50
|
|
3.831E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C99400-TF00 |
16.80
|
|
1.026E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C99500 |
13.70
|
|
1.258E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C99700 |
3.00
|
|
5.747E-07
|
MHASM2
|
resistivity
converted from conductivity |
| C99750 |
2.00
|
|
8.621E-07
|
MHASM2
|
resistivity
converted from conductivity |
| Deoxidized (Annealed) |
85.00
|
4.930E+07
|
2.028E-08
|
CSNDT
|
|
| Electrolytic Tough Pitch (Annealed) |
101.00
|
5.858E+07
|
1.707E-08
|
CSNDT
|
|
| Copper 70%, Nickel 30% |
4.50
|
2.610E+06
|
3.831E-07
|
ECTM
|
|
| Copper 90%, Nickel 10% |
9.74
|
5.647E+06
|
1.771E-07
|
ECT
|
|
| Cupro - Nickel 30% |
4.60
|
2.668E+06
|
3.748E-07
|
CSNDT
|
|
| |
|
|
|
|
|
| Beryllium Copper |
|
|
|
|
|
| Beryllium Copper, Cond. "A" |
17.00
|
9.860E+06
|
1.014E-07
|
CSNDT
|
|
| Beryllium Copper, Cond. At |
21.00
|
1.218E+07
|
8.210E-08
|
CSNDT
|
|
| Beryllium Copper 21C |
20.00
|
|
8.620E-04
|
MHASM2
|
|
| Beryllium Copper Nickel 72C |
43.00
|
|
4.000E-03
|
MHASM2
|
|
| |
|
|
|
|
|
| Brass |
|
|
|
|
|
| Admiralty Brass |
24.00
|
1.392E+07
|
7.184E-08
|
ECTM
|
|
| Admiralty Metal (Annealed) |
24.60
|
1.427E+07
|
7.009E-08
|
CSNDT
|
|
| Aluminum Brass (Annealed) |
23.00
|
1.334E+07
|
7.496E-08
|
CSNDT
|
|
| Cartridge (Annealed) |
28.00
|
1.624E+07
|
6.158E-08
|
CSNDT
|
|
| High Strength Yellow |
12.00
|
6.960E+06
|
1.437E-07
|
CSNDT
|
|
| Leaded Naval (Annealed) |
26.00
|
1.508E+07
|
6.631E-08
|
CSNDT
|
|
| Leaded Semi Red |
18.00
|
1.044E+07
|
9.579E-08
|
CSNDT
|
|
| Leaded Yellow |
25.00
|
1.450E+07
|
6.897E-08
|
CSNDT
|
|
| Low (Annealed) |
32.00
|
1.856E+07
|
5.388E-08
|
CSNDT
|
|
| Low Leaded (Annealed) |
26.00
|
1.508E+07
|
6.631E-08
|
CSNDT
|
|
| Naval (Annealed) |
26.00
|
1.508E+07
|
6.631E-08
|
CSNDT
|
|
| Red (Annealed) |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
| Yellow (Annealed) |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
| Aluminum Brass (Annealed) |
23.00
|
1.334E+07
|
7.496E-08
|
CSNDT
|
|
| |
|
|
|
|
|
| Bronze |
|
|
|
|
|
| Commercial (Annealed) |
44.00
|
2.552E+07
|
3.918E-08
|
CSNDT
|
|
| Commercial Leaded |
42.00
|
2.436E+07
|
4.105E-08
|
CSNDT
|
|
| Leaded Tin |
14.00
|
8.120E+06
|
1.232E-07
|
CSNDT
|
|
| Leaded Tin Bearing |
11.00
|
6.380E+06
|
1.567E-07
|
CSNDT
|
|
| Manganese Bronze (Annealed) |
24.00
|
1.392E+07
|
7.184E-08
|
CSNDT
|
|
| 1.25% Phos. Grade E |
48.00
|
2.784E+07
|
3.592E-08
|
CSNDT
|
|
| 5% Phos. Grade A |
18.00
|
1.044E+07
|
9.579E-08
|
CSNDT
|
|
| 8% Phos. Grade C |
13.00
|
7.540E+06
|
1.326E-07
|
CSNDT
|
|
| 10% Phos. Grade D |
11.00
|
6.380E+06
|
1.567E-07
|
CSNDT
|
|
| |
|
|
|
|
|
| Aluminum Bronze |
|
|
|
|
|
| Aluminum - Bronze |
14.00
|
8.120E+06
|
1.232E-07
|
CSNDT
|
|
| 5% Aluminum (Annealed) |
17.50
|
1.015E+07
|
9.852E-08
|
CSNDT
|
|
| 10% Aluminum (Annealed) |
12.60
|
7.308E+06
|
1.368E-07
|
CSNDT
|
|
| |
|
|
|
|
|
| Silicon Bronze |
|
|
|
|
|
| Silicon Bronze, Type A (Annealed) |
7.00
|
4.060E+06
|
2.463E-07
|
CSNDT
|
|
| Silicon Bronze, Type B (Annealed) |
12.00
|
6.960E+06
|
1.437E-07
|
CSNDT
|
|
|
|
|
|
|
|